| Property |
Thickness |
Value |
Units |
Test |
|
OPTICAL
|
| Haze |
92 |
0.3 |
% |
ASTM D1003 |
| Haze |
142 |
0.3 |
% |
ASTM D1003 |
| Haze |
200 |
0.4 |
% |
ASTM D1003 |
| Haze |
300 |
0.4 |
% |
ASTM D1003 |
| Haze |
400 |
0.5 |
% |
ASTM D1003 |
| Haze |
500 |
0.6 |
% |
ASTM D1003 |
| Haze |
700 |
1.0 |
% |
ASTM D1003 |
| TLT |
92 |
88.8 |
% |
ASTM D1003 |
| TLT |
142 |
88.7 |
% |
ASTM D1003 |
| TLT |
200 |
88.7 |
% |
ASTM D1003 |
| TLT |
300 |
88.5 |
% |
ASTM D1003 |
| TLT |
400 |
88.3 |
% |
ASTM D1003 |
| TLT |
500 |
88.0 |
% |
ASTM D1003 |
| TLT |
700 |
87.0 |
% |
ASTM D1003 |
|
|
|
PHYSICAL
|
| C.O.F. (dynamic) |
92 - 700 |
0.4 |
|
ASTM D1894 |
| Elongation at Break MD |
92 - 200 |
150 |
% |
ASTM D882A |
| Elongation at Break MD |
300 - 700 |
150 |
% |
ASTM D882A |
| Elongation at Break TD |
92 - 200 |
100 |
% |
ASTM D882A |
| Elongation at Break TD |
300 - 700 |
100 |
% |
ASTM D882A |
| Tensile Strength MD |
92 - 200 |
28,000 |
psi |
ASTM D882A |
| Tensile Strength MD |
300 - 700 |
28,000 |
psi |
ASTM D882A |
| Tensile Strength TD |
92 - 200 |
36,000 |
psi |
ASTM D882A |
| Tensile Strength TD |
300 - 700 |
36,000 |
psi |
ASTM D882A |
| Yield (nominal) |
92 |
21,800 |
in˛/lb |
|
| Yield (nominal) |
142 |
14,000 |
in˛/lb |
|
| Yield (nominal) |
200 |
9,900 |
in˛/lb |
|
| Yield (nominal) |
300 |
6,600 |
in˛/lb |
|
| Yield (nominal) |
400 |
5,000 |
in˛/lb |
|
| Yield (nominal) |
500 |
4,000 |
in˛/lb |
|
| Yield (nominal) |
700 |
2,800 |
in˛/lb |
|
| Yield Strength MD |
92 - 200 |
14,000 |
psi |
ASTM D882A |
| Yield Strength MD |
300 - 700 |
14,000 |
psi |
ASTM D882A |
| Yield Strength TD |
92 - 200 |
14,000 |
psi |
ASTM D882A |
| Yield Strength TD |
300 - 700 |
14,000 |
psi |
ASTM D882A |
|
|
|
THERMAL
|
| Shrinkage MD (190°C) |
92 - 200 |
2.5 |
% |
Unrestrained @190°C/5 min |
| Shrinkage MD (190°C) |
300 - 700 |
2.5 |
% |
Unrestrained @ 190°C/5 min |
| Shrinkage TD (190°C) |
92 - 200 |
1.0 |
% |
Unrestrained @190°C/5 min |
| Shrinkage TD (190°C) |
300 - 700 |
1.0 |
% |
Unrestrained @ 190°C/5 min |
|