| Property |
Thickness |
Value |
Units |
Test |
|
OPTICAL
|
| Gloss 45 Degrees |
92 |
38 |
% |
ASTM D523 |
| Gloss 60 Degrees |
92 |
40 |
% |
ASTM D523 |
| Haze |
48 |
51 |
% |
ASTM D1003 |
| Haze |
75 |
66 |
% |
ASTM D1003 |
| Haze |
92 |
73 |
% |
ASTM D1003 |
| Haze |
142 |
78 |
% |
ASTM D1003 |
| Haze |
200 |
95 |
% |
ASTM D1003 |
| Haze |
300-500 |
97 |
% |
ASTM D1003 |
| TLT |
48 |
80 |
% |
ASTM D1003 |
| TLT |
75 |
79 |
% |
ASTM D1003 |
| TLT |
92 |
78 |
% |
ASTM D1003 |
| TLT |
142 |
76 |
% |
ASTM D1003 |
| TLT |
200 |
70 |
% |
ASTM D1003 |
| TLT |
300-500 |
67 |
% |
ASTM D1003 |
|
|
|
PHYSICAL
|
| C.O.F. (dynamic) |
|
0.30 |
|
ASTM D1894 (A-B) |
| Elongation at Break TD |
|
100 |
% |
ASTM D882-83 (23°C at 50% RH, strain rate 50% min) |
| Tensile Strength MD (break) |
|
24,900 |
psi |
ASTM D882-83 (23°C at 50% RH, strain rate 50% min) |
| Tensile Strength TD (break) |
|
30,600 |
psi |
ASTM D882-83 (23°C at 50% RH, strain rate 50% min) |
| Yield Strength MD 5% |
|
14,500 |
psi |
ASTM D882A |
| Yield Strength TD 5% |
|
15,000 |
psi |
ASTM D882A |
|
|
|
THERMAL
|
| Coefficient of Thermal Expansion - MD |
|
19X10E-6 |
cm/cm/°C |
Between 20-50°C |
| Coefficient of Thermal Expansion - TD |
|
16X10E-6 |
cm/cm/°C |
Between 20-50°C |
| Shrinkage MD (190°C) |
48 |
3.0 |
% |
Unrestrained @ 190°C/5 min |
| Shrinkage MD (190°C) |
75-142 |
3.0 |
% |
Unrestrained @ 190°C/5 min |
| Shrinkage MD (190°C) |
200-500 |
3.0 |
% |
Unrestrained @190°C/5 min |
| Shrinkage TD (190°C) |
48 |
3.0 |
% |
Unrestrained @ 190°C/5 min |
| Shrinkage TD (190°C) |
75-142 |
0.0 |
% |
Unrestrained @ 190°C/5 min |
| Shrinkage TD (190°C) |
200-500 |
3.0 |
% |
Unrestrained @ 190°C/5 min |
| Upper Melt Temperature |
|
491-500 |
°F |
ASTM E794-85 |